抄録
This paper reports the texture development in Si3N4 by strong magnetic field alignment (SMFA), using slip casting of α-Si 3N4 raw powder (SN-E10) and pressureless sintering. The texture of β-Si3N4 in the green and sintered bodies was characterized by X-ray diffraction analysis (XRD) and scanning electron microscopy (SEM). The a, b-axis and c-axis aligned β-Si3N 4 has been obtained by the static and rotating magnetic field of 12 T, respectively. The β-seed addition and prolonged sintering both enhance the texture, but the former is more efficient. This work suggests an efficient SMFA strategy of producing highly textured β-Si3N4, particularly the unidirectionally c-axis aligned β-Si3N 4 by seeding the α-raw powder using the less-agglomerated β-phase particles.
本文言語 | English |
---|---|
ページ(範囲) | 871-874 |
ページ数 | 4 |
ジャーナル | Key Engineering Materials |
巻 | 368-372 PART 1 |
DOI | |
出版ステータス | Published - 2008 |
外部発表 | はい |
ASJC Scopus subject areas
- 材料科学(全般)
- 材料力学
- 機械工学